摘要
研究了PPO、SBS、EPDM对HIPS的增韧效果,结果表明HIPS/PPO/SBS/EPDM的组成比例为60/30/5/5时,能使HIPS合金悬臂梁缺口冲击强度达到32.8kJ/m2。通过添加磷系复合阻燃剂,HIPS合金阻燃性能达到FV-O级,烟密度等级67.35,悬臂梁缺口冲击强度10.1kJ/m2,实现了无卤阻燃;添加对环境友好的溴系复合阻燃剂,HIPS合金氧指数可高达32%,具有良好的综合性能。
Toughening effects of PPO, SBS, EPDM on HIPS were studied. The results indicated when the proportion of HIPS/PPO/SBS/EPDM alloy was 70/30/5/5, the notched Izod impact strength was up to 32.83kJ/m^2. Adding the phosphorus composite flame-retardants system, the flammability and notched Izod impact strength of the HIPS alloy could be up to FV-0 and 10.lkJ/m^2 respectively, and the smoking density rank was 67.35. The non-halogen flame retardant HIPS came true. The bromine flame-retardants system was friendly to the environment; it could improve the oxygen index of HIPS alloy up to 32% with excellent balanced property.
出处
《合成材料老化与应用》
2005年第3期11-12,16,共3页
Synthetic Materials Aging and Application
基金
科技部科研院所技术开发研究专项资金(NCSTE-2002-JKZX-095)