摘要
本文通过生产实践得出,含 Mn18—28%,(Mn+Fe)38—48%的铁锰矿都可在高炉中生产富锰渣。利用高磷高铁的铁锰矿和低磷高硅贫锰矿进行配矿入炉,采用自然碱度酸性渣操作,控制渣中SiO_2含量在24—30%,可以炼出低磷低铁优质富锰渣。
According to the production practice,the iron-manganese ores containing 18-28% Mn or 38-48%(Mn+Fe) Can be used to produce rich manganese slag in BF.Using proportioned burden of iron-manganese ore with high phosphorus and iron contedts and low-grade manganese ore with low phosphorus content and high sinicon content,operating with acid slag of natural basicity and controlling SiO_2 content of 24-30%,in slag the good quality rich Mn slag could be produced.A way of reasonable application of iron-manganese ores with high P and Fe contents and low-grade manganese ores with high si content was made.
出处
《中国锰业》
北大核心
1993年第3期20-24,共5页
China Manganese Industry
关键词
锰矿石
富锰渣
高炉
熔炼
Manganse ore
Manganese-rich Slag
Blast Furnace
Smelting