摘要
由硬脂酸和环氧乙烷聚合生成聚氧乙烯酯,然后,再与硬脂酸单甘酯复配得水溶性浆纱后上蜡。确定工艺条件:聚合反应温度为120±10℃,压力为588~784kPa,时间为3h,复配温度为80~90℃。产品收率为98%以上,产品性能达到进口产品水平。该工艺适合中小型化工厂生产。
Polymerizing stearic acid with epoxy ethane,polyoxyethylene ester was synthesized ,then, it was composited with monostearin,thus,a waxapplied to the starching yarn was prepared.The determined process conditions were that, polymerization temperature,120±10℃;pressue,588~784 kPa:reaction period,3h; composition temperature,80~90℃,Yield of tlie produetwas above 98%,and properties of the product achieved quality level of imported one,The process was suitable for middle and small-sized plants.
出处
《河北化工》
1995年第4期1-4,共4页
Hebei Chemical Industry
关键词
水溶性
浆纱后上蜡
硬脂酸
环氧乙烷
制备
蜡
water-soluble wax on the starching yarn, stearic acid, epoxyethane,monostearin, polymerization, composition