摘要
采用Brabender转矩流变仪研究炭黑N330填充型粉末NR[P(NR/N330)]的密炼机塑炼工艺特性。结果表明,P(NR/N330)的塑炼温度低于块状NR;P(NR/N330)适宜的塑炼工艺条件为:温度90℃,转子转速70r.min-1,时间5min。
The mastication conditions of black N330-filled powdered NR[-P(NR/N330)] in internal mixer were investigated by using Brabender torque rheometer. The results showed that the mastication temperature of P(NR/N330) was lower than that of block NR;the suitable mastication conditions of P(NR/N330) were as follows.mastication temperature at 90 ℃ ,rotor speed at 70 r · min^-1 ,and mastication time of 5 rain.
出处
《橡胶工业》
CAS
北大核心
2007年第9期556-559,共4页
China Rubber Industry
基金
广东省自然科学基金资助项目(031366
0400016)
华南理工大学自然科学基金资助项目(324-E5040160)