摘要
根据惯性约束聚变靶材料研究的需要采用自悬浮定向流技术制备了金属纳米Fe粉,通过透射电子显微镜和X射线衍射分析技术研究了颗粒的形貌、粒度和相组成。结果表明,所制备的纳米Fe粉为规则的球状颗粒,其粒径分布在30~70nm之间,在空气中颗粒表面有氧化膜生成,其氧化产物为Fe3O4。
Fe nanoparticles were prepared by flow-levitation method for physical doping of ICF target materials. The morphologies, granularities and structures of Fe particles were investigated by TEM, XRD techniques. The results show that the particles prepared by this means are spherical and the particle size can be controlled availably in 30-70 nm. In addition, it is discovered by XRD techniques that there appeared Fe3O4 oxide film generated in the air, adhering to the surface of the nanoparticles.
出处
《强激光与粒子束》
EI
CAS
CSCD
北大核心
2008年第2期244-246,共3页
High Power Laser and Particle Beams
基金
中国工程物理研究院基金资助课题(20060860)
高温高密度等离子体物理国防科技重点实验室基金资助课题(9140C6805020607)
关键词
纳米Fe粉
物理掺杂
自悬浮定向流法
相结构
ICF靶材料
Fe nanopowder
Flow-levitation method
Physical doping
Appearance structure
ICF target materials