摘要
Leaching of lowgrade refractory tungsten ore was carried out through mechanical activation. The effect of temperature, amount of Na2CO3, addition of NaOH, ratio of liquid to solid and leaching time on the recovery of WO3 was studied. The WO3 recovery upto 96%~99% has been achieved when the tungsten ore was digested by soda not more than three times stiochiometric amount at 185~195 ℃ for 10~20 h. The WO3 recovery can increase 10%~15% compared to that of conventional soda autoclave process.