摘要
建立了钢渣中多种矿质元素的检测方法。钢渣样品经HNO3-HF-HClO4消化,采用电感耦合等离子体质谱(ICP-MS)法检测钢渣中10种矿质元素。该方法的检出限为0.002~6.68μg.g-1,加标回收率为78.8%~105.7%,相对标准偏差(RSD)为0.68%~8.29%。该方法具有简便、快速、准确等特点,可用于钢渣中矿质元素的分析。
Inductive coupled plasma mass spectrometry (ICP-MS) was used to analyze the contents of 10 mineral elements in slag. After digested completely by HNO3-HF-HC104, these samples were determined using the internal method. The recoveries for spiking samples were 78.8%--105.7%, and the relative standard deviations were 0.68%--8.29%. The range of the detection limits of elements was 0.002--6.68 μg.g^-1. The proposed method is simple, rapid and accurate, and could be used to analyze mineral elements in the slag.
出处
《安徽农业大学学报》
CAS
CSCD
北大核心
2011年第1期87-90,共4页
Journal of Anhui Agricultural University
基金
国家十一.五科技支撑计划课题(2008BADA9B08)资助