摘要
根据北方某低品位铁磷矿中铁、磷、钛的赋存状态,采用重选、强磁选或重选—强磁选的联合流程进行综合回收利用试验研究.试验结果表明:先浮选后磁选流程可取得了较好的选矿指标,铁精矿TFe品位66.12%、回收率TFe 23.20%(磁性铁回收率93.98%),磷精矿P2O5品位38.65%、回收率96.23%,钛铁精矿TiO2品位44.62%、回收率44.62%.
According to the condition of a north low-grade iron phosphorus ore in hard,the phosphorus,the titanium tax saves,the authors use the gravity separation,the strong magnetic separation or the gravity separation-strong magnetic separation union flow conducts the synthesis recycling experimental study.Test result shows: After first flotation process,the magnetic separation flow might obtain the good dressing target,hard ore concentrate TFe quality score 66.12%,returns-ratio TFe 23.20%(magnetic hard returns-ratio 93.98%),phosphorus ore concentrate P2O5 quality score 38.65%,returns-ratios 96.23%,ferrotitanium ore concentrate TiO2 quality score 44.62%,returns-ratios 44.62%.
出处
《武汉工程大学学报》
CAS
2011年第3期65-68,共4页
Journal of Wuhan Institute of Technology
关键词
低品位
铁磷钛
综合回收
low-grade
iron-phosphorus-titanium
comprehensive recycling