摘要
本文阐述了在武钢第一炼钢厂条件下生产高碳钢采用高碳出钢工艺的研究及应用情况。通过对过程炉渣、过程温度与倒渣时机等工艺参数的有效控制,可以在吹炼终点熔池[C]达0.3%~0.8%的情况下,使熔池[P]控制在0.015%以内,从而达到降低生产成本、提高钢水纯净度的目的。
This article sets forth the researches and application of producing high-carbon steel adopting high carbon taping technology in the No.1 stealmaking plant in Wu steel.By controlling the process parameters such as process slag,process temperature and deslag time,the[P]in bath can be controlled below 0.015%,under the condition that [C]in the blowing bath reaches 0.3%~0.8%,thus,to decreace the cost of prodution and increase the purification of liquid water.
出处
《河南冶金》
2006年第S1期52-57,共6页
Henan Metallurgy
关键词
高碳低磷钢
倒渣
高碳出钢
去磷
high carbon blow phosphorus steel skim high carbon tape dephosphorus