摘要
针对彝良难选鲕状赤褐铁矿进行了系统的选矿试验研究,采用强磁选—反浮选及选择性絮凝浮选脱泥—反浮选均可以得到较好的选别指标:在强磁选—反浮选小型闭路试验中可以得到铁品位54.70%、回收率达79.44%、含磷仅0.17%的铁精矿;在选择性絮凝后浮选脱泥—反浮选的工艺流程中可以得到铁品位54.63%、铁回收率达77.62%、含磷仅0.15%的铁精矿。
The systematic experimental research was carried out on a refractory oolitic hematite limonite ore in Yiliang, good index were obtained both by flowsheet of "high -intensity magnetic concentration- reverse floatation" and " floatation desliming after selective flocculation -reverse floatation". An iron concentrate containing 54.70% TFe bearing 0.17% P with a recovery of 79. 44% was obtained by the former flowsheet, and an iron concentrate containing 54.63% TFe bearing 0. 15%P with a recovery of 77.62% was obtained by the latter flowsheet.
出处
《矿产保护与利用》
2012年第2期37-41,共5页
Conservation and Utilization of Mineral Resources
关键词
鲕状赤褐铁矿
提铁降磷
选择性絮凝
强磁选
反浮选
oolitic hematite limonite ore
iron improvement and phosphorus reduction
the selective flocculation
high -intensity magnetic concentration