摘要
莱钢265m2烧结机采用预热混合料、强化制粒、配加0.5%蛇纹石、控制焦粉配比4.50%等措施,解决了料层透气性差、垂直烧结速度慢等问题,实现了厚度为750mm的厚料层烧结工艺,并保证了烧结矿的产量和质量,降低固体燃耗1kg/t。
By preheating mixed material, intensifying granulation, adding serpentine of 0.5% and controlling coke powder proportion of 4.5%, the 265 m2 sintering machine in Laiwu Steel realized deep-bed sintering process with the thickness of 750 mm. The poor bed permeability, slow vertical sintering speed and other problems were solved, ensuring the yield and quality of the sinter and reducing solid fuel consumption by 1 kg/t.
出处
《山东冶金》
CAS
2012年第5期20-21,24,共3页
Shandong Metallurgy
关键词
厚料层烧结技术
透气性
烧结速度
蛇纹石
固体燃耗
deep-bed sintering process
permeability
sintering speed
serpentine
solid fuel consumption