摘要
采用浮选工艺对河南某低品位钾长石矿进行了综合利用研究,试验结果表明,采用原矿—磨矿—脱泥—长石石英分离浮选—强磁选的选矿工艺流程,可获得产率58.30%、K2O+Na2O=12.12%的长石产品,同时可得到产率为19.94%、SiO297.12%石英产品,实现了少尾工艺,从而为该矿资源的合理开发做出了较好的选矿评价。
A low - grade potash feldspar in Helaan had been studied using flotation method and new flotation reagent. Based on small- scale experimental research, a principle flowsheet of raw ore - grinding -desliming -flotation (separation of feldspar and quartz) -high intensity magnetic separation had been developed. This technology finally output potash feldspar concentrate with a yield of 58.30% ,the K2O + Na2O grade being 12.12% ; and quartz product with a yield of 19.94%, containing 97.12% SiO2. A process of less tailings had been truly realized. A good processing evaluation was made for the reasonable exploitation of this mineral resource.
出处
《矿产保护与利用》
2012年第5期34-38,共5页
Conservation and Utilization of Mineral Resources
基金
国家科技支撑计划项目(编号:2011BAB03B01)
地质调查评价专项(编号:1212011120306)
关键词
低品位钾长石
浮选
综合利用
low- grade potash feldspar
flotation
comprehensive utilization