摘要
通过优化电炉出钢喷炭粉、调整脱氧制度、选择合适时机的钙处理、采用合理的调硫工艺等一系列措施.经“UHP+IJ+VD+CC”工艺流程,批量生产出全氧质量分数≤20×10-6,硫化物夹杂级别≤2.0级的汽车用含硫齿轮钢fS含量范围在0.017%-0.035%)。
By taking a series of measures such as spraying carbon powder during EAF tapping, adjusting deoxydation process, calcium treatment at appropriate stage, reasonable sulfur adjustment process and stirring before casting, The sulfur-beating pinion steel for automotive with total [O]≤20×10-6 and sulfide inclusion ≤2.0 was produced through "UHP+LF+VD+CC"(sulfur content was controlled within 0.017%-0.035%).
出处
《铸造技术》
CAS
北大核心
2013年第5期590-592,共3页
Foundry Technology
关键词
含硫齿轮钢
纯净度
含S量
sulfur-bearing pinion steels
clean level
S content