摘要
应用热力学稳定性好的氧化钙耐火材料,提高精炼温度,强化碳脱氧的热力学和动力学条件。
A melting technique of carbon deoxidization of VIM (vacuum induction melting) was discussed. Inconel 718 alloy, M17F alloy and iron were used as the testing materials. Applying thermodynamic stable CaO refractory as the melting crucible and increasing refining temperature, the thermodynamic and kinetic conditions of carbon deoxidization were strengthened. The results show that the oxygen content of Inconel 718 is decreased from 0.0025% to 0.0006%, M17F from 0.0025% to 0.0009%, and iron from 0.0055% to 0.0025%.
出处
《材料研究学报》
EI
CAS
CSCD
北大核心
2001年第3期275-278,共4页
Chinese Journal of Materials Research