期刊文献+

Al_(87)Ni_(10)Zr_3纳米非晶材料的形成及其晶化行为 被引量:5

Formation and Crystallization Behavior of Nanocrystal Amorphous in Melt Spun Al_(87) Ni_(10) Zr_3 Alloy
下载PDF
导出
摘要 采用单辊旋淬技术制备快速凝固Al87Ni10 Zr3 合金。利用X -射线衍射、透射电子显微镜分析研究了合金薄带的急冷态和各退火态的显微组织。结果表明 :急冷态组织为非晶态和纳米晶的复合体 ,晶态组织是细小的Al基固溶体 (60~ 80nm)和Al3 (Ni ,Zr)相 (<2 0nm) ,非晶的形成取决于合金成分和凝固速率。低温 (2 0 0℃ )退火导致了非晶的晶化 ;高温 (3 5 0℃ ,2h)退火 ,过饱和Al基固溶体和Al3 (Ni ,Zr)相将析出或转变为亚稳L12 -Al3 Zr和Al3 Ni相 ,L12 -Al3 Zr相尺寸非常细小 (<2 0nm) ,退火时间达到 2 0h ,L12-Al3 Zr相尺寸仍无明显变化 。 Rapidly solidified Al 87 Ni 10 Zr 3 alloy was prepared by single roller melt spinning. As spun and as annealed state, the microstructure of the ribbons was examined by X ray diffraction(XRD) and transmission election microscopy(TEM). It was shown that the as spun alloy consisted of amorphous state and crystallized grains containing fine aluminum solid solution(60~80 nm in size) and Al 3(Ni,Zr) phase(<20 nm in size). The formation of amorphous state depended on composition and solidification velocity. Low temperature(200 ℃) heat treatment led to crystallization of amorphous. At higher temperature(350 ℃ at 2 hours), the super saturated solid solution Al precipitated and Al 3(Ni,Zr) phase transformed to a metastable L 12 Al 3Zr phase, less than 20 nm in size, which was found to be very stable even up to 20 hours at 350 ℃.
出处 《矿冶工程》 CAS CSCD 北大核心 2002年第1期98-100,共3页 Mining and Metallurgical Engineering
基金 安徽省教委自然科学基金项目 (2 0 0 0j1 1 72 )
关键词 快速凝固 Al87NiZr3合金 Ll2-Al3Zr相 显微组织 品化 铝基非晶态合金 rapid solidification Al 87 Ni 10 Zr 3 alloy amorphous state L 12 Al 3Zr phase microstructure
  • 相关文献

参考文献4

二级参考文献14

  • 1仝兴存,沈宁福,МАНОВВ.П..快速凝固Al-RE-Ni非晶合金的显微结构及热稳定性分析[J].金属学报,1993,29(1). 被引量:1
  • 2小池精一.-[J].日本金属学会志,1992,56(8):394-394.
  • 3[1]Fores F H,Kim Y W,Hehmann F.J.Metal.,1987,40(8):14
  • 4[3]Miller W S,Palmer I G.Met.Powder Rep.,1986,41(10):761
  • 5[4]Lieblich M,Canuana G.Mater Sci.Tech.,1996,22(1):25
  • 6[5]Chuang M S,Scr.Metall.Mater.,1994,31(9):1259
  • 7[6]Zedalis M S,Fine M E.Met.Trans.,1986,17A:2187
  • 8[7]Chen Y C,Fine M E.Acta.Met.,1990,38:771
  • 9Chung M S,Scr Metall Mater,1995年,33卷,12期,1999页
  • 10Chung M S,Scr Metall Mater,1994年,31卷,9期,1259页

共引文献16

同被引文献91

  • 1苏勇,陈翌庆,丁厚福,郑玉春.Al_(91)Ni_7Y_2纳米非晶复合材料晶化的研究[J].兵器材料科学与工程,2000,23(4):12-15. 被引量:4
  • 2卢柯.非晶态合金向纳米晶体的相转变[J].金属学报,1994,30(1). 被引量:50
  • 3刘鸿凌,王飒飒,鲁圣国,张良莹,姚熹.非晶态SiO_2中纳米ZnS的量子尺寸效应与非线性光学效应[J].科学通报,1996,41(4):367-369. 被引量:2
  • 4卢柯,周飞.纳米晶体材料的研究现状[J].金属学报,1997,33(1):99-106. 被引量:114
  • 5[1]GLEITER H.Nanocrystalline materials[J].Prog in Mater Sci,1989,33:223-227.
  • 6[2]YOSHIZAWA Y,OGUMA S.New Fe-based soft magnetic alloys composed fultrafine grainstructure[J].J Appl Phys,1988,64(10):6044-6060.
  • 7[6]INOUE A,FAN C,SAIDA J,et al.High-strength Zr-based bulk amorphous alloys containing nanocrys talline and nanoquasicrystalline particles[J].Science and Technology of Advanced Materials,2000,(1):73-86.
  • 8[8]HASIAK M,ZBROSZCZYK J,OLSZEESKI J,et al.Effect of cooling rate on magnectic properties of amorphous and nanocrystalline Fe73.5 Cu1 Nb3 Si15.5 B7 alloy[J].J Magn Magn Mater,2000,215-216:410-412.
  • 9[9]INOUE A,CHERA K.Crystallization of aluminium-basedmetallicglasses:processes and kinetics[J].Jpn J Appl Phys,1988,27(3):280-287.
  • 10[10]INOUE A,KIMURA H.Fabrications and mechanical properties of bulk amorphous,nanocrystalline,nanoquasicrystalline alloys in aluminum-based system[J].J Light Metals,2001,(1):31-41.

引证文献5

二级引证文献22

相关作者

内容加载中请稍等...

相关机构

内容加载中请稍等...

相关主题

内容加载中请稍等...

浏览历史

内容加载中请稍等...
;
使用帮助 返回顶部