摘要
在实验室条件下对承钢含钛高炉渣进行了脱硫过程的动力学研究,确定其脱硫的相关动力学参数。结果发现:在温度一定时,铁水中脱硫量和时间的延长而降低。由于铁水的脱硫反应属于二级反应,硫在熔渣中的扩散成了脱硫过程的限制性环节,熔渣的脱硫能力与炉温成正比,并且在试验中的到硫在熔渣中的扩散活化能为ED=127.04kJ/mol。
The kinetics of desulfurization process of bearing steel titanium bearing blast furnace slag was carried out under laboratory conditions to determine the relevant parameters,the desulfurization. Results:in a certain tempera-ture,hot metal desulphurization extension in quantity and time and reduce. The desulfurization reaction of molten i-ron belongs to two order reaction,diffusion of sulfur in slag into the restricted link of desulfurization process,desulfu-rization capacity of slag is proportional to furnace temperature,and spread to the sulfur in test in slag activation en-ergy is ED = 127. 04 kJ/ mol.
出处
《河北联合大学学报(自然科学版)》
CAS
2014年第3期27-29,共3页
Journal of Hebei Polytechnic University:Social Science Edition
基金
国家科技支撑计划(2012BAE09B00)
关键词
钛渣
脱硫动力学
传质系数
活化能
Titanium slag
desulphurization kinetics
mass transfer coefficient
activation energy