摘要
通过比表面积和孔体积、SEM、XPS表征手段,对新鲜Pd Cl2-Cu Cl2/AC催化剂和反应后失活催化剂进行了比较。试验结果表明,催化剂表面金属铜向内部迁移,而钯基本不变,致使催化剂比表面积和孔体积都减小。从而发现了催化剂失活的另一原因。
It studied in comparing with the fresh and deactived catalys of Pd Cl2-Cu Cl2/AC according to specific surface area, aperture volumes, XEM and XPS. Another result of catalyst deactivation was discovered. It was revealed that Cu coule be transferred from the surface of catalyst to the inner but Pd could be not which caused to the diminishing of specific surface area and aperture volumes.
出处
《广东化工》
CAS
2015年第16期110-111,共2页
Guangdong Chemical Industry
基金
濮阳职业技术学院自然科学研究项目(2015PYZYZR07)
关键词
碳酸二甲酯
金属迁移
催化剂失活
dimethyl carbonate
metal migration
catalyst deactivation