摘要
采用β(β″)-Al2O3固体电解质管组装固体电解质电池Pt|Sb2O5,NaSbO3‖β(β″)-Al2O3‖NaCrO2,Cr2O3|Pt和Pt|TeO2,Na2TeO3‖β(β″)-Al2O3‖NaCrO2,Cr2O3|Pt。测量不同温度下达到平衡时的电池反应电动势,计算NaSbO3和Na2TeO3生成自由能,建立生成自由能与温度的关系。得到在700~1300K范围内NaSbO3生成自由能与温度的关系为:ΔGθNaSbO3=-655.88+0.2039T±4.10(kJ/mol);在700~1100K范围内Na2TeO3生成自由能与温度的关系为ΔGθNa2TeO3=-700.35+0.0519T±9.29(kJ/mol)。
The solid electrolyte cells Ptl Sb2O5, NaSbO3 β 13 ( β")-A1203 II NaCrO2, Cr2O3 I Pt and Pt I TeO2, Na2TeO3 II 13 (β")-A12 O3 II NaCrO2, Cr2 O31Pt were assembled using △ (β")-A12O3 as solid electrolyte, and the for- mation free energies of NaSbO3 and Na2TeO3 were calculated by measuring the electromotive force (EMF) of cells. The relationship between formation free energy and temperature (700 - 1300 K) for NaSbO3 can be described as △GN,shO3 = -655.88 +0. 2039T +4. 10 (kJ/mol) and that for Na2TeO3 in the temperature range of 700 ~ 1100 K can be described as △GNO2TeO3 = -700.35 +0. 0519T +9.29 (kJ/mol).
出处
《矿冶》
CAS
2015年第4期22-26,共5页
Mining And Metallurgy
基金
国家自然科学基金重点项目(51234009)