摘要
某镀金同轴连接器能够通过48 h中性盐雾试验,但组装为连接线运输到日本客户处时却存在氧化发黑现象。分析认为是PVC(聚氯乙烯)材质的包装材料在运输过程中受热分解产生的HCl腐蚀了镀层。在PVC包装前增加PE(聚乙烯)材质的包装,该问题得到解决。
A gold-plated coaxial connector was able to pass a 48-hour neutral salt spray test,but it was found to be oxidized and blackened after being assembled to be a connection line and transported to Japanese customers.The analysis results showed that the packaging made of PVC(polyvinyl chloride)was decomposed by heat during transportation,resulting in the corrosion of gold coating by the decomposition product i.e.HCl.The problem was solved by wrapping with PE(polyethylene)and PVC films successively.
作者
樊磊
FAN Lei(Wanma Group Special Electron Cable Co.,Ltd.,Hangzhou 311300,China)
出处
《电镀与涂饰》
CAS
CSCD
北大核心
2019年第7期321-323,共3页
Electroplating & Finishing
基金
浙江省省级工业新产品(20172270)
关键词
连接器
镀金
包装
氧化
聚氯乙烯
热分解
connector
gold plating
packaging
oxidation
polyvinyl chloride
thermal decomposition