摘要
以砂磨机为粉碎设备 ,得到对绢云母进行超细粉碎的最佳工艺条件 :磨矿时间 6h ,矿浆质量分数 40 % ,助磨剂用量 0 .2 0 %。应用三种改性剂对超细绢云母进行干法改性并将改性后的产品充填于丁苯橡胶中 ,通过改性预评价及充填丁苯橡胶性能测试 ,得到铝酸脂改性效果最佳。
Best processing conditions of ultra fine grinding of sericite with sand mill were suggested as follows: grinding time 6h, slurry density 40%, addition quantity of grinding aid agent 0.20%. Three kinds of modifying agents were tested by dry method. The physical properties of modified sericite were measured with several different methods. The results showed that the best modifying agent was coupling agent of organic aluminate.
出处
《化工矿物与加工》
CAS
北大核心
2003年第9期14-16,共3页
Industrial Minerals & Processing
关键词
绢云母
超细粉碎
表面改性
丁苯橡胶
sericite
ultra fine grinding
surface modification
SBR