The normal compression tests on intact samples and artificial joints with different saw-tooth shape under cyclic loading and half-sine waves of different frequencies were performed by using Instron1342 servo-controlle...The normal compression tests on intact samples and artificial joints with different saw-tooth shape under cyclic loading and half-sine waves of different frequencies were performed by using Instron1342 servo-controlled material testing machine. The specimens were made artificially with mortar. The loading frequency ranged from 0.005 Hz to 0.1 Hz. The experimental results show that joint closure curves are non-linear and concave up. The stress-deformation curves under cyclic loading exhibit hysteresis and permanent set that diminish rapidly and keep constant finally on successive cycles. Normal displacement successively decreases from the joint J1 to J2, to J3 under the same normal loads regardless of frequency. Considering the loading frequency effect, normal displacement of joint J1 decreases with increasing the loading frequency except that the loading frequency is 0.05 Hz. Normal displacement of joint J2 increases with increasing the loading frequency. Normal displacement of joint J3 increases with increasing the loading frequency when the frequency ranges from 0.005 Hz to 0.05 Hz. Its normal displacement, however, becomes least when the loading frequency is 0.1 Hz.展开更多
The healing behavior of shrinkage cavity inside the cast Ti6Al4V alloy during hot isostatic pressing(HIP)was investigated experimentally by interrupted hot isostatic pressing tests.The X-ray micro computed tomography ...The healing behavior of shrinkage cavity inside the cast Ti6Al4V alloy during hot isostatic pressing(HIP)was investigated experimentally by interrupted hot isostatic pressing tests.The X-ray micro computed tomography was used to record the morphology changes before and after hot isostatic pressing.The two-dimensional geometry obtained by the microCT scan was used in simulation to study the evolution of the real shrinkage cavity during hot isostatic pressing.Shrinkage cavities,shrinkage porosity and small gas pores can be effectively eliminated under proper HIP conditions.The two-dimensional morphology in the simulation results agrees well with the experimental results.This study reveals that plastic deformation,creep and diffusion are the main mechanisms of cavity closure during hot isostatic pressing.In addition,the simplified elliptical pores with aspect ratios at different positions were used to replace the real pores to further study the factors affecting the position of dimples after HIP by simulation.It is found that the position of the dimples mainly depends on the aspect ratio of the elliptical pore and the distance between the pore surface and the external surface of the geometric model.展开更多
基金Projects(50490274 50490272) supported by the National Natural Science Foundation of ChinaProject(2002CB412703) supported by theNational Basic Research Program of China
文摘The normal compression tests on intact samples and artificial joints with different saw-tooth shape under cyclic loading and half-sine waves of different frequencies were performed by using Instron1342 servo-controlled material testing machine. The specimens were made artificially with mortar. The loading frequency ranged from 0.005 Hz to 0.1 Hz. The experimental results show that joint closure curves are non-linear and concave up. The stress-deformation curves under cyclic loading exhibit hysteresis and permanent set that diminish rapidly and keep constant finally on successive cycles. Normal displacement successively decreases from the joint J1 to J2, to J3 under the same normal loads regardless of frequency. Considering the loading frequency effect, normal displacement of joint J1 decreases with increasing the loading frequency except that the loading frequency is 0.05 Hz. Normal displacement of joint J2 increases with increasing the loading frequency. Normal displacement of joint J3 increases with increasing the loading frequency when the frequency ranges from 0.005 Hz to 0.05 Hz. Its normal displacement, however, becomes least when the loading frequency is 0.1 Hz.
基金financially supportedby the National Key Research and Development Program of China(No.2020YFB1710100)the State Key Laboratory of Special Rare Metal Materials(Contract No.SKL2018K004)+1 种基金the Northwest Rare Metal Materials Research Institute Ningxia Co.,Ltd.,the National Natural Science Foundation of China(Grant No.51475181 and 51775205)the AECC Beijing Institute of Aeronautical Materials。
文摘The healing behavior of shrinkage cavity inside the cast Ti6Al4V alloy during hot isostatic pressing(HIP)was investigated experimentally by interrupted hot isostatic pressing tests.The X-ray micro computed tomography was used to record the morphology changes before and after hot isostatic pressing.The two-dimensional geometry obtained by the microCT scan was used in simulation to study the evolution of the real shrinkage cavity during hot isostatic pressing.Shrinkage cavities,shrinkage porosity and small gas pores can be effectively eliminated under proper HIP conditions.The two-dimensional morphology in the simulation results agrees well with the experimental results.This study reveals that plastic deformation,creep and diffusion are the main mechanisms of cavity closure during hot isostatic pressing.In addition,the simplified elliptical pores with aspect ratios at different positions were used to replace the real pores to further study the factors affecting the position of dimples after HIP by simulation.It is found that the position of the dimples mainly depends on the aspect ratio of the elliptical pore and the distance between the pore surface and the external surface of the geometric model.