Hydroxyapatite-graft-poly(D-lactide)(HA-g-PDLA)was synthesized by ring-opening polymerization with HA as initiator and stannous octanoate(Sn(Oct)2)as catalyst.Thermogravimetric analysis(TGA)and Fourier transform infra...Hydroxyapatite-graft-poly(D-lactide)(HA-g-PDLA)was synthesized by ring-opening polymerization with HA as initiator and stannous octanoate(Sn(Oct)2)as catalyst.Thermogravimetric analysis(TGA)and Fourier transform infrared spectroscopy(FUR)results indicate that PDLA chains are successfully grafted onto HA particles by covalent bond.Under two different processing temperatures(190 and 230℃),the effect of the grafted PDLA chains on the crystallization behavior of poly(L-lactide)/HA-g-PDLA(PLLA/HA-g-PDLA)composite was investigated in the current study,comparing to neat PLLA and its four composites(PLLA/HA,PLLA/HA-g-PLLA,PLLA/PDLA,and PLLA/HA/PDLA).The crystallization rate of PLLA/HA-g-PDLA composite is highly enhanced comparing to PLLA,PLLA/HA and PLLA/HA-g-PLLA composites in which there are no stereocomplex(SC)crystallites.In addition,when the processing temperature rises from 190℃ to 230℃,the acceleration of PLLA crystallization in PLLA/HA-g-PDLA composite is not influenced so much as other composites containing SC crystallites,such as PLLA/HA/PDLA or PLLA/PDLA.The differential scanning calorimetry(DSC)results demonstrate that even without SC crystallites,the crystallization of PLLA can still be accelerated a lot in this composite.This may be related to the interaction between the grafted PDLA chains and the amorphous PLLA chains in PLLA/HA-g-PDLA composite.The isothermal crystallization kinetics studies indicate that the nature of nucleation and crystal growth of PLLA/HAg-PDLA composite are more likely 3D crystalline growth with heterogeneous nucleation mode,which are different from PLLA or other composites.This investigation could shed new light on the application of PLLA/HA composites.展开更多
In the version of this Article originally published,Fig.7(f)was con fused with Fig.4(f).The corrected version of Fig.7 is provided below.This graphical amendment does not affect the analyses,and additional text correc...In the version of this Article originally published,Fig.7(f)was con fused with Fig.4(f).The corrected version of Fig.7 is provided below.This graphical amendment does not affect the analyses,and additional text corrections are not needed.展开更多
基金the National Natural Science Foundation of China(Nos.51603005 and 51973010)Beijing Natural Science Foundation(No.2182052).
文摘Hydroxyapatite-graft-poly(D-lactide)(HA-g-PDLA)was synthesized by ring-opening polymerization with HA as initiator and stannous octanoate(Sn(Oct)2)as catalyst.Thermogravimetric analysis(TGA)and Fourier transform infrared spectroscopy(FUR)results indicate that PDLA chains are successfully grafted onto HA particles by covalent bond.Under two different processing temperatures(190 and 230℃),the effect of the grafted PDLA chains on the crystallization behavior of poly(L-lactide)/HA-g-PDLA(PLLA/HA-g-PDLA)composite was investigated in the current study,comparing to neat PLLA and its four composites(PLLA/HA,PLLA/HA-g-PLLA,PLLA/PDLA,and PLLA/HA/PDLA).The crystallization rate of PLLA/HA-g-PDLA composite is highly enhanced comparing to PLLA,PLLA/HA and PLLA/HA-g-PLLA composites in which there are no stereocomplex(SC)crystallites.In addition,when the processing temperature rises from 190℃ to 230℃,the acceleration of PLLA crystallization in PLLA/HA-g-PDLA composite is not influenced so much as other composites containing SC crystallites,such as PLLA/HA/PDLA or PLLA/PDLA.The differential scanning calorimetry(DSC)results demonstrate that even without SC crystallites,the crystallization of PLLA can still be accelerated a lot in this composite.This may be related to the interaction between the grafted PDLA chains and the amorphous PLLA chains in PLLA/HA-g-PDLA composite.The isothermal crystallization kinetics studies indicate that the nature of nucleation and crystal growth of PLLA/HAg-PDLA composite are more likely 3D crystalline growth with heterogeneous nucleation mode,which are different from PLLA or other composites.This investigation could shed new light on the application of PLLA/HA composites.
文摘In the version of this Article originally published,Fig.7(f)was con fused with Fig.4(f).The corrected version of Fig.7 is provided below.This graphical amendment does not affect the analyses,and additional text corrections are not needed.