Mixed Al-Si and Al-Cu powders were investigated as insert layers to reactive diffusion bond SiCp/6063 metal matrix composite (MMC). The results show that SiCp/6063 MMC joints bonded by the insert layers of the mixed...Mixed Al-Si and Al-Cu powders were investigated as insert layers to reactive diffusion bond SiCp/6063 metal matrix composite (MMC). The results show that SiCp/6063 MMC joints bonded by the insert layers of the mixed Al-Si and Al-Cu powders have a dense joining layer of high quality. The mass transfer between the bonded materials and insert layers during bonding leads to the hypoeutectic microstructure of the joining layers bonded by both the mixed Al-Si and Al-Cu powders with eutectic composition. At fixed bonding time (temperature), the shear strength of the joints by both insert layers of the mixed Al-Si and Al-Cu powders increases with increasing the bonding temperature (time), but get maxima at bonding temperature 600℃ (time 90 min).展开更多
Mixed Al-Si and Al-Si-SiC powders were employed as insert layers to reactive diffusion bond SiCp/6063 MMC (metal matrix composites). The results show that SiCp/6063 MMC joints bonded by the insert layer of the mixed...Mixed Al-Si and Al-Si-SiC powders were employed as insert layers to reactive diffusion bond SiCp/6063 MMC (metal matrix composites). The results show that SiCp/6063 MMC joints bonded by the insert layer of the mixed Al-Si powder have a dense joining layer with a typical hypoeutectic microstructtn'e. Using the mixed Al-Si-SiC powder as the insert layer, SiCp/6063 MMC can be reactive diffusion bonded by a composite joint. Because of the SiC segregation, however, there are a number of porous zones in the joining layer, which results in the bad shear strength of the joints reactive diffusion bonded by the insert layer of the mixed A1-Si- SiC powder, even lower than that of the joints reactive diffusion bonded by the insert layer of the mixed Al-Si powder. Ti and Mg added in the insert layers obviously improve the strength of the joints reactive diffusion bonded by the insert layer of the mixed Al- Si-SiC powder, especially, Mg has a more obvious effect.展开更多
基金the National Natural Science Foundation of China under grant No.50175004
文摘Mixed Al-Si and Al-Cu powders were investigated as insert layers to reactive diffusion bond SiCp/6063 metal matrix composite (MMC). The results show that SiCp/6063 MMC joints bonded by the insert layers of the mixed Al-Si and Al-Cu powders have a dense joining layer of high quality. The mass transfer between the bonded materials and insert layers during bonding leads to the hypoeutectic microstructure of the joining layers bonded by both the mixed Al-Si and Al-Cu powders with eutectic composition. At fixed bonding time (temperature), the shear strength of the joints by both insert layers of the mixed Al-Si and Al-Cu powders increases with increasing the bonding temperature (time), but get maxima at bonding temperature 600℃ (time 90 min).
基金This work was financially supported by the National Natural Science Foundation of China (No. 50175004)
文摘Mixed Al-Si and Al-Si-SiC powders were employed as insert layers to reactive diffusion bond SiCp/6063 MMC (metal matrix composites). The results show that SiCp/6063 MMC joints bonded by the insert layer of the mixed Al-Si powder have a dense joining layer with a typical hypoeutectic microstructtn'e. Using the mixed Al-Si-SiC powder as the insert layer, SiCp/6063 MMC can be reactive diffusion bonded by a composite joint. Because of the SiC segregation, however, there are a number of porous zones in the joining layer, which results in the bad shear strength of the joints reactive diffusion bonded by the insert layer of the mixed A1-Si- SiC powder, even lower than that of the joints reactive diffusion bonded by the insert layer of the mixed Al-Si powder. Ti and Mg added in the insert layers obviously improve the strength of the joints reactive diffusion bonded by the insert layer of the mixed Al- Si-SiC powder, especially, Mg has a more obvious effect.