In order to study the effects of the process parameters on springback and section deformation, a sensitivity analysis model was established based on the combination use of the multi-parameter sensitivity analysis meth...In order to study the effects of the process parameters on springback and section deformation, a sensitivity analysis model was established based on the combination use of the multi-parameter sensitivity analysis method and the springback/section deformation prediction finite element model, and by using this model the sensitivities of the springback and the section deformation to process parameters were analyzed and compared. The results show that the most sensitive process conditions for springback angle are the boost speed and the pressure of pressure die, and the most sensitive process condition for section deformation is the number of cores. When the clamp force, the boost speed and the pressure of pressure die are utilized to control section deformation, the effect of these process parameters on springback should be considered. When the process parameters are mainly used to control springback, the effect of these process parameters on the section deformation should be always considered.展开更多
The mechanical characteristics of the weld joint were investigated by tensile test, microstructure test, and microhardness test. The welded tube NC bending tests were carried out to evaluate the weld on the formabilit...The mechanical characteristics of the weld joint were investigated by tensile test, microstructure test, and microhardness test. The welded tube NC bending tests were carried out to evaluate the weld on the formability of the QSTE340 welded tube. The results show that the wall thinning degree, cross-sectional deformation and springback angle increase significantly as the weld line is located on the outside of the bend compared with that located on the middle and inside, and the welded tubes produce nearly identical performance as the weld line is located on the middle and inside. The wall thickening degree decreases much as the weld line is located on the inside of the bend. So the welded tube can acquire good bending formability as the weld line is located in the region away from the outside of the bend.展开更多
基金Project (50975235) supported by the National Natural Science Foundation of ChinaProject (B08040) supported by the 111 Project
文摘In order to study the effects of the process parameters on springback and section deformation, a sensitivity analysis model was established based on the combination use of the multi-parameter sensitivity analysis method and the springback/section deformation prediction finite element model, and by using this model the sensitivities of the springback and the section deformation to process parameters were analyzed and compared. The results show that the most sensitive process conditions for springback angle are the boost speed and the pressure of pressure die, and the most sensitive process condition for section deformation is the number of cores. When the clamp force, the boost speed and the pressure of pressure die are utilized to control section deformation, the effect of these process parameters on springback should be considered. When the process parameters are mainly used to control springback, the effect of these process parameters on the section deformation should be always considered.
基金Supported by National Natural Science Foundation of China (No. 50875216)
文摘The mechanical characteristics of the weld joint were investigated by tensile test, microstructure test, and microhardness test. The welded tube NC bending tests were carried out to evaluate the weld on the formability of the QSTE340 welded tube. The results show that the wall thinning degree, cross-sectional deformation and springback angle increase significantly as the weld line is located on the outside of the bend compared with that located on the middle and inside, and the welded tubes produce nearly identical performance as the weld line is located on the middle and inside. The wall thickening degree decreases much as the weld line is located on the inside of the bend. So the welded tube can acquire good bending formability as the weld line is located in the region away from the outside of the bend.