TC4 titanium alloy was friction stir welded using a W-Re pin tool,and the defect-free weld was produced with proper welding parameters.The joint consists of stir zone,heat affected zone and base material.The stir zone...TC4 titanium alloy was friction stir welded using a W-Re pin tool,and the defect-free weld was produced with proper welding parameters.The joint consists of stir zone,heat affected zone and base material.The stir zone is characterized by equiaxed dynamically recrystallized α phases and transformed β phases with fine α+β lamellar microstructure.The microstructure of the heat-affected zone is similar to that of the base material,but there is an increase in the volume fraction of β.Transverse tensile strength of the joint is 92% that of the base material,and the joint is fractured in the stir zone and the fracture surface possesses typical plastic fracture characteristics.The stir zone is the weakest part of the joint,through which the tensile characteristics of the TC4 joint can be explained.展开更多
Hot stamping 22MnB5 steel plate with ultra-high strength has been widely used for body structural members in consideration of automobile safety and lightweight.This paper presents a verification program of simulating ...Hot stamping 22MnB5 steel plate with ultra-high strength has been widely used for body structural members in consideration of automobile safety and lightweight.This paper presents a verification program of simulating and testing pole impact in order to verify if the front crossbeam reinforcement assembly can meet the design requirements,reduce the overall vehicle simulation and test cost and shorten the operation period.In the same condition,the simulation proved conforming to the design requirements;however,the bumper cracked at the impacting point in the course of pole impact test.The analysis of the crack by optical microscope,Vickers and scanning electron microscope indicates that mixture of ferrite,bainite and martensite was produced in the weld heat-affected zone of the 340/590DP tow hook holder and the 22MnB5 front crossbeam;therefore,their hardness and mechanical property were reduced obviously,so that they fractured when impacted.No welding process with continuous weld but spot welding or other bonding method may be employed for the reason that the capacity of the 22MnB5 steel plate in the weld heat-affected zone was reduced obviously.展开更多
基金Project(2010CB731704) supported by the National Basic Research Program of ChinaProject supported by the Program of Excellent Team in Harbin Institute of Technology, China
文摘TC4 titanium alloy was friction stir welded using a W-Re pin tool,and the defect-free weld was produced with proper welding parameters.The joint consists of stir zone,heat affected zone and base material.The stir zone is characterized by equiaxed dynamically recrystallized α phases and transformed β phases with fine α+β lamellar microstructure.The microstructure of the heat-affected zone is similar to that of the base material,but there is an increase in the volume fraction of β.Transverse tensile strength of the joint is 92% that of the base material,and the joint is fractured in the stir zone and the fracture surface possesses typical plastic fracture characteristics.The stir zone is the weakest part of the joint,through which the tensile characteristics of the TC4 joint can be explained.
基金"Twelfth Five-year Plan"for Sci & Tech Research of China(No.2011BAG03B02No.2011BAG03B06)
文摘Hot stamping 22MnB5 steel plate with ultra-high strength has been widely used for body structural members in consideration of automobile safety and lightweight.This paper presents a verification program of simulating and testing pole impact in order to verify if the front crossbeam reinforcement assembly can meet the design requirements,reduce the overall vehicle simulation and test cost and shorten the operation period.In the same condition,the simulation proved conforming to the design requirements;however,the bumper cracked at the impacting point in the course of pole impact test.The analysis of the crack by optical microscope,Vickers and scanning electron microscope indicates that mixture of ferrite,bainite and martensite was produced in the weld heat-affected zone of the 340/590DP tow hook holder and the 22MnB5 front crossbeam;therefore,their hardness and mechanical property were reduced obviously,so that they fractured when impacted.No welding process with continuous weld but spot welding or other bonding method may be employed for the reason that the capacity of the 22MnB5 steel plate in the weld heat-affected zone was reduced obviously.