The microstructural evolution and phase transformations during partial remelting of in-situ Mg2Sip/AM60B composite modified by SiC and Sr were investigated. The results indicate that SiC and Sr are effective for refi...The microstructural evolution and phase transformations during partial remelting of in-situ Mg2Sip/AM60B composite modified by SiC and Sr were investigated. The results indicate that SiC and Sr are effective for refining primary α-Mg grains and Mg2Si particles. After being partially remelted, a semisolid microstructure with small and spheroidal primary α-Mg particles can be obtained. The microstructural evolution during partial remelting can be divided into four stages: the initial rapid coarsening, structural separation, spheroidization and final coarsening, which are essentially caused by the phase transformations of β→α, α+β→L and α→L, α→L, and α→L and L→α, respectively. The Mg2Si particles have not obvious effect on the general microstructural evolution steps, but can slower the evolution progress and change the coarsening mechanism. During partial remelting, Mg2Si particles first become blunt and then become spheroidal because of melting of their edges and corners, and finally are coarsened owing to Ostwald ripening.展开更多
AM60B magnesium alloy was refined by MgCO3 and its microstmcturat evolution was investigated during partial remelting. The results indicate that MgCO3 is an effective grain refiner for AM60B alloy and can decrease the...AM60B magnesium alloy was refined by MgCO3 and its microstmcturat evolution was investigated during partial remelting. The results indicate that MgCO3 is an effective grain refiner for AM60B alloy and can decrease the grain size from 329 pm of the unrefined alloy to 69 μm. A semisolid microstructure with small and spheroidal primary particles can be obtained after being partially remelted. The microstructure evolution can be divided into four steps: the initial rapid coarsening, structure separation, spheroidization and final coarsening. Correspondingly, these four steps result from the phase transformations of β→α, α+β→L and α→L, α→L and two reverse reactions of α→L and L→α, respectively. One spheroidal primary particle in the semisolid microstmcture usually originates one dendrite in the as-cast microstructure. The variation of primary particle size with holding time does not obey the LSW law, Dt^3-Do^3=Kt, after the semisolid system is in its solid-liquid equilibrium state. Longer heating duration makes the primary particles more globular, but it makes their size larger at the same time.展开更多
The billets of AM60 alloy, prepared with self-inoculation method, were partially remelted into semisolid state. Effects of process parameters on remelting microstructure of semisolid billet were investigated. Experime...The billets of AM60 alloy, prepared with self-inoculation method, were partially remelted into semisolid state. Effects of process parameters on remelting microstructure of semisolid billet were investigated. Experimental results show that the solid particles obtained with self-inoculation method are in smaller grain size and globular shape after partial remelting, compared with those prepared with other casting methods. In the optimized process conditions, the average size of solid particles of partially remelted billet is 65 μm, and the shape factor is 1.12. The process parameters, i.e. pouting temperature, addition amount of self-inoculants, and the slope angle of multi-stream mixing cooling chalmel have influence on the microstructure of partially remelted billet. The optimized temperature is from 680 ℃ to 700 ℃, addition amount of self-inoculants is between 5% and 7% (mass fraction), slope angle of multi-stream mixing cooling channel is between 30° and 45°, with which the dendritic microstructure of as-cast billet can be avoided, and the size of solid particles ofremelted billet is reduced.展开更多
基金Project(G2010CB635106)supported by the National Basic Research Program of ChinaProject(NCET-10-0023)supported by the Program for New Century Excellent Talents in University of ChinaProject supported by the Program for Hongliu Outstanding Talents of Lanzhou University of Technology,China
文摘The microstructural evolution and phase transformations during partial remelting of in-situ Mg2Sip/AM60B composite modified by SiC and Sr were investigated. The results indicate that SiC and Sr are effective for refining primary α-Mg grains and Mg2Si particles. After being partially remelted, a semisolid microstructure with small and spheroidal primary α-Mg particles can be obtained. The microstructural evolution during partial remelting can be divided into four stages: the initial rapid coarsening, structural separation, spheroidization and final coarsening, which are essentially caused by the phase transformations of β→α, α+β→L and α→L, α→L, and α→L and L→α, respectively. The Mg2Si particles have not obvious effect on the general microstructural evolution steps, but can slower the evolution progress and change the coarsening mechanism. During partial remelting, Mg2Si particles first become blunt and then become spheroidal because of melting of their edges and corners, and finally are coarsened owing to Ostwald ripening.
基金Project(G2007CB613706) supported by the National Basic Research Program of China
文摘AM60B magnesium alloy was refined by MgCO3 and its microstmcturat evolution was investigated during partial remelting. The results indicate that MgCO3 is an effective grain refiner for AM60B alloy and can decrease the grain size from 329 pm of the unrefined alloy to 69 μm. A semisolid microstructure with small and spheroidal primary particles can be obtained after being partially remelted. The microstructure evolution can be divided into four steps: the initial rapid coarsening, structure separation, spheroidization and final coarsening. Correspondingly, these four steps result from the phase transformations of β→α, α+β→L and α→L, α→L and two reverse reactions of α→L and L→α, respectively. One spheroidal primary particle in the semisolid microstmcture usually originates one dendrite in the as-cast microstructure. The variation of primary particle size with holding time does not obey the LSW law, Dt^3-Do^3=Kt, after the semisolid system is in its solid-liquid equilibrium state. Longer heating duration makes the primary particles more globular, but it makes their size larger at the same time.
基金Project(2007CB613700) supported by the National Basic Research Program of ChinaProject(50964010) supported by the National Natural Science Foundation of ChinaProject(090WCGA894) supported by the International S&T Cooperation Program of Gansu Province,China
文摘The billets of AM60 alloy, prepared with self-inoculation method, were partially remelted into semisolid state. Effects of process parameters on remelting microstructure of semisolid billet were investigated. Experimental results show that the solid particles obtained with self-inoculation method are in smaller grain size and globular shape after partial remelting, compared with those prepared with other casting methods. In the optimized process conditions, the average size of solid particles of partially remelted billet is 65 μm, and the shape factor is 1.12. The process parameters, i.e. pouting temperature, addition amount of self-inoculants, and the slope angle of multi-stream mixing cooling chalmel have influence on the microstructure of partially remelted billet. The optimized temperature is from 680 ℃ to 700 ℃, addition amount of self-inoculants is between 5% and 7% (mass fraction), slope angle of multi-stream mixing cooling channel is between 30° and 45°, with which the dendritic microstructure of as-cast billet can be avoided, and the size of solid particles ofremelted billet is reduced.