For the high sulfur refractory gold concentrate with 41.82%sulfur and 15.12 g/t gold,of which 82.11%was wrapped in sulfide,a well-controlled stirring tank leaching was carried out to improve the bio-oxidation efficien...For the high sulfur refractory gold concentrate with 41.82%sulfur and 15.12 g/t gold,of which 82.11%was wrapped in sulfide,a well-controlled stirring tank leaching was carried out to improve the bio-oxidation efficiency.Results show that bio-oxidation pretreatment can greatly improve the gold recovery rate of high-sulfur refractory gold concentrate,and at the optimum pH 1.3 in this study,compared with the process without pH control,the oxidation rate of sulfur increased from 79.31%to 83.29%,while the recovery rate of gold increased from 76.54%to 83.23%;under this condition the activity of mixed culture could be sustained and the formation of jarosite could diminish.The results also displayed that for the high sulfur refractory gold concentrate,the recovery of gold is positively correlated with the oxidation rate of sulfur,and the recovery rate of gold increases with the increase of sulfur oxidation rate within a certain range.展开更多
Mexican copper ore is a mixed ore containing mainly copper oxide and some copper sulfide that responds well to flotation. The joint techniques of flotation and leaching were studied. The results indicate that an ore c...Mexican copper ore is a mixed ore containing mainly copper oxide and some copper sulfide that responds well to flotation. The joint techniques of flotation and leaching were studied. The results indicate that an ore containing 19.01% copper could be obtained at a recovery ratio of 35.02% by using sodium sulfide and butyl xanthate flotation. Over 83.33% of the copper oxide can be recovered from the railings by leaching in suitable conditions, such as 1 h stirring at a temperature around 25 ℃with a mixing speed of S00 r/min, an H2SO4 concentration of 1.0 mol/L and a mass ratio of the ore-slurry-liquid to solid (mL/ms) of 3. The overall yield of refined ore after flotation and leaching is over 89.18% of the copper, which is much better than sole flotation or leaching. A copper product containing more than 99.9% copper was obtained by using the process: flotation-agitation leaching- solvent extraction-electro-winning.展开更多
基金Projects(51704028,51574036)supported by the National Natural Science Foundation of ChinaProject supported by Program for Key Laboratory of Biohydrometallurgy of Ministry of Education Foundation,China。
文摘For the high sulfur refractory gold concentrate with 41.82%sulfur and 15.12 g/t gold,of which 82.11%was wrapped in sulfide,a well-controlled stirring tank leaching was carried out to improve the bio-oxidation efficiency.Results show that bio-oxidation pretreatment can greatly improve the gold recovery rate of high-sulfur refractory gold concentrate,and at the optimum pH 1.3 in this study,compared with the process without pH control,the oxidation rate of sulfur increased from 79.31%to 83.29%,while the recovery rate of gold increased from 76.54%to 83.23%;under this condition the activity of mixed culture could be sustained and the formation of jarosite could diminish.The results also displayed that for the high sulfur refractory gold concentrate,the recovery of gold is positively correlated with the oxidation rate of sulfur,and the recovery rate of gold increases with the increase of sulfur oxidation rate within a certain range.
基金Projects 50604016 supported by the National Natural Science Foundation of China2007BAB22B01 by the 11th Five-Year Plan of National Science and Technology of China
文摘Mexican copper ore is a mixed ore containing mainly copper oxide and some copper sulfide that responds well to flotation. The joint techniques of flotation and leaching were studied. The results indicate that an ore containing 19.01% copper could be obtained at a recovery ratio of 35.02% by using sodium sulfide and butyl xanthate flotation. Over 83.33% of the copper oxide can be recovered from the railings by leaching in suitable conditions, such as 1 h stirring at a temperature around 25 ℃with a mixing speed of S00 r/min, an H2SO4 concentration of 1.0 mol/L and a mass ratio of the ore-slurry-liquid to solid (mL/ms) of 3. The overall yield of refined ore after flotation and leaching is over 89.18% of the copper, which is much better than sole flotation or leaching. A copper product containing more than 99.9% copper was obtained by using the process: flotation-agitation leaching- solvent extraction-electro-winning.