Al2O3 - SiC - C castables with pelletized graphite addition of 0. 2%, 4% or 6% (by mass, the same hereinafter ) were prepared using brown fused corundum (8 - 5, 5 - 3 and 3 - 1 mm ) , dense fused corundum ( ≤1 a...Al2O3 - SiC - C castables with pelletized graphite addition of 0. 2%, 4% or 6% (by mass, the same hereinafter ) were prepared using brown fused corundum (8 - 5, 5 - 3 and 3 - 1 mm ) , dense fused corundum ( ≤1 and 0. 045 mm) and SiC ( ≤1 and ≤0. 064 mm) its main starting materials with mass ratio of aggregate: matrix = 71: 29, 2% silicon powder and 0. 4% B4C as antioxidants, and pelletized graphite as carbon source, Effect of pelletized graphite addition on physical properties, oxidation resistance, slag resistance arid thermal shock resistance of Al2O3 -SiC- C eastables was researched. The results show that: with the in.crease of pelletized graphite addition, the required water amount of castables increases, the bulk density and strength reduce; with 4% pelletized graphite, the eastable performs the best oxidation resistance; the increase of graphite is beneficial to the improvement of slag penetration resistance and corrosion resistance; with 6% pelletized graphite, the thermal shock resistance is the best.展开更多
The influences of adding steel fibres of different lengths up to 3 volume percentages, on the rheological behaviour of an alumina-magnesia-extruded graphite pellet containing castables have been studied using a rheome...The influences of adding steel fibres of different lengths up to 3 volume percentages, on the rheological behaviour of an alumina-magnesia-extruded graphite pellet containing castables have been studied using a rheometer. Free-flow measurements have shown that the flow is severely affected by increasing the length of steel fibres. The calculated values of rheological constants indicate that 19 mm and 25 mm fibre up to 2 volume percentage is permitted while one volume percentage of 50 mm fibres severely degrades the rheology of the castable.展开更多
文摘Al2O3 - SiC - C castables with pelletized graphite addition of 0. 2%, 4% or 6% (by mass, the same hereinafter ) were prepared using brown fused corundum (8 - 5, 5 - 3 and 3 - 1 mm ) , dense fused corundum ( ≤1 and 0. 045 mm) and SiC ( ≤1 and ≤0. 064 mm) its main starting materials with mass ratio of aggregate: matrix = 71: 29, 2% silicon powder and 0. 4% B4C as antioxidants, and pelletized graphite as carbon source, Effect of pelletized graphite addition on physical properties, oxidation resistance, slag resistance arid thermal shock resistance of Al2O3 -SiC- C eastables was researched. The results show that: with the in.crease of pelletized graphite addition, the required water amount of castables increases, the bulk density and strength reduce; with 4% pelletized graphite, the eastable performs the best oxidation resistance; the increase of graphite is beneficial to the improvement of slag penetration resistance and corrosion resistance; with 6% pelletized graphite, the thermal shock resistance is the best.
文摘The influences of adding steel fibres of different lengths up to 3 volume percentages, on the rheological behaviour of an alumina-magnesia-extruded graphite pellet containing castables have been studied using a rheometer. Free-flow measurements have shown that the flow is severely affected by increasing the length of steel fibres. The calculated values of rheological constants indicate that 19 mm and 25 mm fibre up to 2 volume percentage is permitted while one volume percentage of 50 mm fibres severely degrades the rheology of the castable.