A hydrometallurgical process for refractory gold-bearing arsenosulfide concentrates at ambient temperature and pressure was presented, including fine grinding with intensified alkali-leaching (FGIAL), enhanced agita...A hydrometallurgical process for refractory gold-bearing arsenosulfide concentrates at ambient temperature and pressure was presented, including fine grinding with intensified alkali-leaching (FGIAL), enhanced agitation alkali-leaching (EAAL), thiosulfate leaching and displacement. Experimental results on a refractory gold concentrate showed that the total consumption of NaOH in alkaline leaching is only 41% of those theoretically calculated under the conditions of full oxidization for the same amount of arse- nides and sulfides transformed into arsenates and sulfates, and 72.3% of gold is synchro-dissoluted by thiosulfate self-generated during alkaline leaching. After alkaline leaching, thiosulfate leaching was carried out for 24 h. The dissolution of gold is increased to 91.9% from 4.6% by cyanide without the pretreatment. The displacement of gold by zinc powder in the solution gets to 99.2%. Due to an amount of thiosulfate self-generated during alkaline leaching, the reagent addition in thiosulfate leaching afterwards is lower than the normal.展开更多
The thiourea leaching of gold from the calcine of gold-bearing arsenical pyrite concentrate of Kangjiawan mine was studied.The effects of the leaching time,the concentrations of thiourea,hydrochloric acid and initial ...The thiourea leaching of gold from the calcine of gold-bearing arsenical pyrite concentrate of Kangjiawan mine was studied.The effects of the leaching time,the concentrations of thiourea,hydrochloric acid and initial ferric ion on the leaching recovery of gold were investigated,and a regressive model has been established,which showed that the concentrations of thiourea and hydrochloric acid were the most important factors,leaching time the second,and concentration of the initial ferric ion the least・Under the optimal conditions,that is,temperature 50℃,the ratio of liquid to solid 4:1,thiourea 12g/L,hydrochloric acid 1 mol/L,and initial ferric ion 1 g/L,the leaching recoveries of gold and silver were more than 81%and 73%,respectively.The increase of silver recovery and the reduction of thiourea consumption could be attained when sodium sulphite was added.展开更多
基金This project was financially supported by the Natural Science Foundation of Liaoning Province of China (No.2001101015) and theFree Study Item of the Institute of Metal Research, Chinese Academy of Sciences (No.AM05-0866)
文摘A hydrometallurgical process for refractory gold-bearing arsenosulfide concentrates at ambient temperature and pressure was presented, including fine grinding with intensified alkali-leaching (FGIAL), enhanced agitation alkali-leaching (EAAL), thiosulfate leaching and displacement. Experimental results on a refractory gold concentrate showed that the total consumption of NaOH in alkaline leaching is only 41% of those theoretically calculated under the conditions of full oxidization for the same amount of arse- nides and sulfides transformed into arsenates and sulfates, and 72.3% of gold is synchro-dissoluted by thiosulfate self-generated during alkaline leaching. After alkaline leaching, thiosulfate leaching was carried out for 24 h. The dissolution of gold is increased to 91.9% from 4.6% by cyanide without the pretreatment. The displacement of gold by zinc powder in the solution gets to 99.2%. Due to an amount of thiosulfate self-generated during alkaline leaching, the reagent addition in thiosulfate leaching afterwards is lower than the normal.
文摘The thiourea leaching of gold from the calcine of gold-bearing arsenical pyrite concentrate of Kangjiawan mine was studied.The effects of the leaching time,the concentrations of thiourea,hydrochloric acid and initial ferric ion on the leaching recovery of gold were investigated,and a regressive model has been established,which showed that the concentrations of thiourea and hydrochloric acid were the most important factors,leaching time the second,and concentration of the initial ferric ion the least・Under the optimal conditions,that is,temperature 50℃,the ratio of liquid to solid 4:1,thiourea 12g/L,hydrochloric acid 1 mol/L,and initial ferric ion 1 g/L,the leaching recoveries of gold and silver were more than 81%and 73%,respectively.The increase of silver recovery and the reduction of thiourea consumption could be attained when sodium sulphite was added.