Effects of cooling rate and 0.25 at.%TiB2 addition on solidification microstructure and mechanical properties of Ti−48Al−2Cr−2Nb alloys fabricated by the investment casting with different thicknesses were studied.The ...Effects of cooling rate and 0.25 at.%TiB2 addition on solidification microstructure and mechanical properties of Ti−48Al−2Cr−2Nb alloys fabricated by the investment casting with different thicknesses were studied.The results show that with the cooling rate increasing from 37 to 2×102 K/s,the solidification path of the studied alloys is unchanged.The grain size of the matrix alloy is refined from 650 to 300μm,while the grain size of Ti−48Al−2Cr−2Nb−TiB2 is reduced from 550 to 80μm.The lamellar spacing of matrix alloy is reduced from 360 to 30 nm with increasing the cooling rate from 37 to 2×102 K/s,while TiB2 addition shows little refinement effect on the lamellar spacing.Ti−48Al−2Cr−2Nb−TiB2 sample under medium cooling rate(69 K/s)exhibits superior microhardness(HV 550)and ultimate tensile strength(570 MPa)among the studied alloys.The refined grain size,lamellar spacing and fine TiB2 particles could account for the favorable mechanical properties of the studied TiB2-containing alloy.The microstructure evolution was discussed in light of cooling rate,constitutional supercooling and borides addition.展开更多
Ti/Cu/Ti laminated composites were fabricated by corrugated rolling(CR) and flat rolling(FR) method.Microstructure and mechanical properties of CR and FR laminated composites were investigated by scanning electron mic...Ti/Cu/Ti laminated composites were fabricated by corrugated rolling(CR) and flat rolling(FR) method.Microstructure and mechanical properties of CR and FR laminated composites were investigated by scanning electron microscopy, numerical simulation methods, peel and tensile examinations. The effect of CR and FR was comparatively analyzed. The results showed that the CR and FR laminated composites exhibited different effective plastic strain distributions of the Ti layer and Cu layer at the interface. The recrystallization texture, prismatic texture and pyramidal texture were developed in the Ti layer by CR, while the R-Goss texture and shear texture were developed in the Cu layer by CR. The typical deformation texture components were developed in the Ti layer and Cu layer of FR laminated composites. The CR laminated composites had higher bond strength, tensile strength and ductility.展开更多
基金This work is supported by the National Natural Science Foundation of China(51904205)Science and Technology Foundation of State Key Laboratory,China(6142909180205)+3 种基金China Postdoctoral Science Foundation(2018M641681)Scientific and Technological Innovation Programs of Higher Education Institutions in Shanxi Province,China(2019L0216)Shanxi Province Science and Technology Major Program,China(20181101008)Natural Science Foundation of Shanxi Province,China(201801D221346,201801D221221).
文摘Effects of cooling rate and 0.25 at.%TiB2 addition on solidification microstructure and mechanical properties of Ti−48Al−2Cr−2Nb alloys fabricated by the investment casting with different thicknesses were studied.The results show that with the cooling rate increasing from 37 to 2×102 K/s,the solidification path of the studied alloys is unchanged.The grain size of the matrix alloy is refined from 650 to 300μm,while the grain size of Ti−48Al−2Cr−2Nb−TiB2 is reduced from 550 to 80μm.The lamellar spacing of matrix alloy is reduced from 360 to 30 nm with increasing the cooling rate from 37 to 2×102 K/s,while TiB2 addition shows little refinement effect on the lamellar spacing.Ti−48Al−2Cr−2Nb−TiB2 sample under medium cooling rate(69 K/s)exhibits superior microhardness(HV 550)and ultimate tensile strength(570 MPa)among the studied alloys.The refined grain size,lamellar spacing and fine TiB2 particles could account for the favorable mechanical properties of the studied TiB2-containing alloy.The microstructure evolution was discussed in light of cooling rate,constitutional supercooling and borides addition.
基金financially supported by the National Key R&D Program of China (No.2018YFA0707300)the Natural Science Foundation of Shanxi Province,China (No.201801D221131)+2 种基金the National Natural Science Foundation of China (Nos.51905372,51904206,51805359,52075359)Shanxi Province Science and Technology Major Project,China (No.20181102011)China Postdoctoral Science Foundation (No.2020M670705)。
文摘Ti/Cu/Ti laminated composites were fabricated by corrugated rolling(CR) and flat rolling(FR) method.Microstructure and mechanical properties of CR and FR laminated composites were investigated by scanning electron microscopy, numerical simulation methods, peel and tensile examinations. The effect of CR and FR was comparatively analyzed. The results showed that the CR and FR laminated composites exhibited different effective plastic strain distributions of the Ti layer and Cu layer at the interface. The recrystallization texture, prismatic texture and pyramidal texture were developed in the Ti layer by CR, while the R-Goss texture and shear texture were developed in the Cu layer by CR. The typical deformation texture components were developed in the Ti layer and Cu layer of FR laminated composites. The CR laminated composites had higher bond strength, tensile strength and ductility.